Technical Data
Commercially Pure Titanium
Unalloyed titanium comes in 4 grades determined by strength and impurity content. Primary uses are for corrosion resistance when high strengths are not needed such as heat exchangers and chemical industry piping systems.
Chemistry Limits | ||||||
All in max % | Grade 1 | Grade 2 | Grade 3 | Grade 4 | ||
O2 | 0.18 | 0.25 | 0.35 | 0.40 | ||
Fe | 0.20 | 0.20 | 0.20 | 0.30 | ||
H2 | 0.015 | 0.015 | 0.015 | 0.015 | ||
C | 0.10 | 0.10 | 0.10 | 0.10 | ||
N2 | 0.03 | 0.03 | 0.05 | 0.05 | ||
Mechanical Properties* | ||||||
Minimum | Grade 1 | Grade 2 | Grade 3 | Grade 4 | ||
Ultimate Tensile Strength - ksi | 35 | 50 | 65 | 80 | ||
Yield Strength - ksi | 25 | 40 | 55 | 70 | ||
Elongation % | 25 | 20 | 18 | 15 |
* ASTM Room Temperature Properties for bar
Physical Properties | ||||
Grade 1 | Grade 2 | Grade 3 | Grade 4 | |
Density (lbs/in3) | 0.163 | 0.163 | 0.163 | 0.164 |
Elastic Modulus (x106 psi) | 14.9 | 14.9 | 14.9 | 15.1 |
Beta Transus Temp (oF) | 1630 | 1675 | 1690 | 1740 |
Weldability | Excellent | Excellent | Good | Good |
Previous: Application of Titanium